Technically reviewed by Vincent, Founder at HEXVARO
Last reviewed · Content updated
Quick answer
Quick answer: material by service zone
Choose the material for the zone first, then the coating. For topside and atmospheric service, carbon or alloy steel with hot-dip galvanizing or a PTFE system is the usual choice. For the splash zone and seawater immersion, stainless grades with a PREN over 40 resist pitting and crevice corrosion. For subsea bolts under cathodic protection, keep hardness low: B7 can reach 35 HRC, and steels above 34 HRC are highly susceptible to hydrogen cracking from CP.
| Service zone | Typical material |
|---|---|
| Topside, marine atmosphere | ASTM A193 B7 studs with A194 2H nuts |
| Splash zone and seawater immersion | Super duplex 2507 (PREN 41) |
| Subsea with cathodic protection | ASTM A193 B7M or A320 L7M, hardness-controlled |
Choose the material by service zone
The project's material selection specification, such as NORSOK M-001 on North Sea projects or the operator's own standard, decides the final choice. The table shows the common pattern buyers see on drawings and purchase orders.
| Service zone | Typical material | Typical coating | Main risk |
|---|---|---|---|
| Topside, marine atmosphere | ASTM A193 B7 studs with A194 2H nuts | Hot-dip galvanized or PTFE over a zinc or phosphate base | Atmospheric corrosion of the coating and threads |
| Splash zone and seawater immersion | Super duplex 2507 (PREN 41) | Usually uncoated | Pitting and crevice corrosion under nuts and washers |
| Subsea with cathodic protection | ASTM A193 B7M or A320 L7M, hardness-controlled | As the project specification states | Hydrogen cracking from cathodic protection |
| Sheltered deck and indoor marine | A4 (316) stainless | Uncoated | Tea staining and crevice corrosion in stagnant salt water |
Stainless grades and PREN
The pitting resistance equivalent number (PREN) ranks how well a stainless steel resists pitting and crevice corrosion in chloride. For austenitic grades it is %Cr + 3.3 × %Mo + 16 × %N; for duplex grades the nitrogen factor is usually taken as 30.
A PREN over 40 is the usual guide for a stainless steel that should resist localised corrosion when fully immersed in seawater. A4 (316) is a good choice in salt air but falls well short of that for immersion, especially in the crevices under nuts and washers.
| Grade | Typical PREN | Marine use |
|---|---|---|
| A2 (304) | 19 | Indoor and sheltered use; not for salt spray |
| A4 (316) | 24 | Marine atmosphere and deck hardware |
| Duplex 2205 | 36 | Higher strength and better chloride resistance than 316 |
| Super duplex 2507 (PREN 41) | 41 | Seawater immersion and splash zone |
B7 vs B7M under cathodic protection
Subsea structures are protected by sacrificial anodes or impressed current. Cathodic protection stops the steel corroding, but it also generates hydrogen at the bolt surface. High-strength, high-hardness bolts absorb that hydrogen and can crack under load. A published review of offshore bolt failures found that steels harder than 34 HRC are highly susceptible, and B7 can reach 35 HRC.
ASTM A193 B7M is the lower-hardness version of B7. Its maximum hardness is 235 HB (99 HRB) against 321 HB (35 HRC) for B7, and every stud in a B7M lot is hardness tested. The trade-off is strength: B7M has a minimum tensile strength of 100 ksi, against 125 ksi for B7 up to 2-1/2 in. NORSOK M-001, as quoted by the US regulator BSEE, caps carbon and low-alloy parts exposed to cathodic protection at 328 HB (35 HRC), and a NACE/AMPP paper reports that low-alloy steel bolting has been limited to 34 HRC in CP systems, so the project specification must state the limit.
| Property | ASTM A193 B7 | ASTM A193 B7M |
|---|---|---|
| Maximum hardness | 321 HB (35 HRC) | 235 HB (99 HRB) |
| Minimum tensile strength, up to 2-1/2 in | 125 ksi | 100 ksi |
| Typical offshore use | Topside flanges and structures | Subsea and sour service where hardness is limited |
Coatings for marine service
- Hot-dip galvanizing: a mean of at least 50 µm of zinc (40 µm local minimum) on parts over 6 mm under ISO 1461, with spun galvanizing of M8–M64 fasteners covered by ISO 10684, the standard choice for topside structural and support bolting. Nuts are tapped oversize, so order bolts and nuts as a set.
- PTFE (fluoropolymer): low friction for controlled torque on flange studs, usually applied over a zinc or phosphate base coat. State the base coat, colour and thickness.
- Electroplated zinc: too thin for offshore service. On hard bolts it also adds hydrogen during plating; ASTM B633 calls for baking above 31 HRC. A zinc-coated, high-hardness bolt set was implicated in a 2012 subsea connector failure in the Gulf of Mexico.
- Uncoated stainless and duplex: no coating needed, but avoid mixing stainless bolts with galvanized or aluminium parts in wet joints without isolation.
What to put in an offshore fastener RFQ
- Service zone for each line: topside, splash zone or subsea, and whether cathodic protection applies.
- Material and grade with the standard (for example ASTM A193 B7 or B7M, A194 2H or 2HM nuts) and any maximum hardness.
- Coating system and thickness, and the coating standard (ISO 10684, ASTM F2329, or the PTFE specification).
- Project specification references such as NORSOK M-001, NACE MR0175 / ISO 15156 for sour service, or an API 20E bolting level.
- Size list, quantities, nut and washer pairing, and the documents you need, such as an EN 10204 3.1 mill test certificate.
What HEXVARO supplies for offshore and marine projects
HEXVARO is a manufacturer. We supply ASTM A193 B7 studs and threaded rod with A194 2H nuts, plain, hot-dip galvanized or PTFE coated, plus hot-dip galvanized threaded rod and custom parts to drawing. MOQ is 500 pcs per size. Lead time is 10 to 15 days from stock and 25 to 30 days for production, shipped from Tianjin, Ningbo, Shanghai or Shenzhen, with an EN 10204 3.1 mill test certificate where available.
B7M, L7M, A4 stainless, duplex and super duplex grades, hardness limits and project specifications such as NORSOK M-001 or NACE MR0175: state them in the RFQ and we confirm before quoting. We do not offer API monogrammed bolting.
Frequently asked questions
What is the best material for offshore fasteners?
It depends on the zone. Galvanized or PTFE-coated B7 studs with 2H nuts are common topside. Super duplex, with a PREN over 40, suits seawater immersion. Subsea bolts under cathodic protection need a hardness-controlled grade such as B7M or L7M.
Is A4 (316) stainless steel good enough for seawater?
A4 performs well in marine air, but its PREN of about 24 is well below the level of about 40 usually needed to resist pitting and crevice corrosion when immersed in seawater.
Why are B7M studs used subsea instead of B7?
Cathodic protection puts hydrogen into the bolt surface. Hard bolts are more likely to crack, and B7 can reach 35 HRC. B7M is limited to 235 HB (99 HRB) and every stud is hardness tested.
Can zinc-plated bolts be used offshore?
Electroplated zinc is too thin for offshore service, and on hard bolts the plating process adds hydrogen. Use hot-dip galvanizing or a PTFE system topside, and follow the project specification subsea.
What is the MOQ for offshore stud bolts from HEXVARO?
The MOQ is 500 pcs per size, and mixed sizes are welcome on one order. B7 studs come with 2H nuts, plain, hot-dip galvanized or PTFE coated. We reply to RFQs within 2 working hours.
Products to this standard
Sources for technical review
- Prevention of failures of high strength fasteners in offshore and subsea applications (Bolt Science review)
- QC-FIT evaluation of connector and bolt failures, Report 2014-01 (BSEE)
- Difference between A193 B7 and B7M (Portland Bolt)
- Corrosion resistance: PREN values (Anzor)
- QC-FIT evaluation of BOP shear ram bolt failures, NORSOK M-001 hardness limit (BSEE, 2017)
- High strength fasteners for subsea, paper 04151 (AMPP / NACE)
- Hot dip galvanized bolts and nuts, ISO 1461 coating thickness (HDGASA)
- ISO 10684:2004 Fasteners — Hot dip galvanized coatings (scope M8–M64)